What is in this article?
- How clay shrinks during drying and firing
- Wet, dry and fired measurements
- Measuring clay shrinkage with a test bar
- Calculating percentage from actual measurements
- Sizing clay for a desired fired dimension
- Inverse calculation and combined stages
- Using the clay shrinkage calculator
- Example mugs, tiles and test-bar record
- Worked examples, practical checks and limitations
- Common mistakes and when to seek expert confirmation
- Frequently asked questions
- How big should I make pottery before firing?
- Why did my pot come out smaller than planned?
- Where do I find my clay's shrinkage?
- Does shrinkage apply to height and thickness too?
- Can I add the drying and firing percentages?
- Why fire test bars at more than one temperature?
- Conclusion
- Sources
Clay gets smaller twice: first as it dries, then again in the kiln. If you have wondered how big to make pottery before firing, or looked for a clay shrinkage calculator or a pottery wet-to-fired size calculator, remember that you have to make a piece bigger while it is wet, and the sum is not as simple as adding the shrinkage percentage. This guide explains wet, dry and fired measurements, how to measure your own clay with a test bar, and how to work out the wet size for a target fired size. Shrinkage varies by clay body, firing temperature and forming method, so treat every number here as an example and test your own clay.
To skip the arithmetic, open the free clay shrinkage calculator.
How clay shrinks during drying and firing
Plastic clay holds water between its particles. As the water leaves, the particles move closer and the piece shrinks while it dries to bone dry. In the kiln the clay sinters and vitrifies and shrinks again. Higher firing temperatures generally give more shrinkage, so clay makers publish a typical total figure for each body at its recommended firing.
Wet, dry and fired measurements
| Stage | What you measure |
|---|---|
| Wet | Length while the clay is still plastic |
| Dry (bone dry) | Length after drying fully, before any firing |
| Fired | Length after the firing you normally use |

Measuring clay shrinkage with a test bar
Roll out a flat bar or tile and scratch a line exactly 100 mm long while the clay is wet. Measure it again when bone dry and after the firing you plan to use for real work. Use the same method you will use for your pieces, whether throwing, hand building or slip casting, because forming method can change shrinkage.
The ceramic materials reference Digitalfire describes a standard shrinkage and absorption test (called SHAB) in the same spirit: roll a bar of plastic clay, press a 10 cm mark into it, dry it, record the length, fire it, then record the length again. Their bars are about 2.5 cm (1 inch) wide, and they make one bar for each temperature to be tested, at minimum the target temperature plus one cone above and one below. They also stress that the point is doing things the same way each time so you can compare your own clays, not to produce an absolute standard result.
Calculating percentage from actual measurements
Shrinkage % = (wet length − fired length) ÷ wet length × 100. Example: a 100.0 mm bar measures 94.0 mm dry and 87.5 mm fired. Drying shrinkage = 6.0%. Firing shrinkage = (94.0 − 87.5) ÷ 94.0 = 6.9%. Total shrinkage = (100 − 87.5) ÷ 100 = 12.5%. Notice that 6.0 + 6.9 is 12.9, not 12.5, because the firing percentage is measured against the dry length. Do not simply add stage percentages; measure the total from wet to fired.
Because sources can use different bases (some measure firing shrinkage from the dry length, some from the wet length), always check which basis a published figure uses before comparing it with your own.
Sizing clay for a desired fired dimension
The shrink factor is 1 − (shrinkage ÷ 100). Fired size = wet size × factor. Wet size needed = target fired size ÷ factor.
Inverse calculation and combined stages
Example (illustrative 12% clay): for a 200 mm plate, wet size = 200 ÷ 0.88 = 227.27 mm. If you instead made it 12% bigger (224 mm), it would fire to 224 × 0.88 = 197.12 mm, nearly 3 mm short. Because shrinkage is linear, the same factor applies to height, width, diameter and wall thickness. Volume changes much more, since it depends on the cube of the size.
Using the clay shrinkage calculator
The clay shrinkage calculator has two parts. The first finds the wet size to make for a fired target, or the fired size of a wet piece, from your shrinkage percentage in mm, cm or inches. The second works out your own clay’s shrinkage from wet, optional dry and fired test-bar lengths.
Example mugs, tiles and test-bar record
- Mug (13% example): a 90 mm fired height needs 90 ÷ 0.87 = 103.45 mm wet.
- Tile (10% example): a 150 mm fired tile needs 150 ÷ 0.90 = 166.67 mm wet.
- Record: note clay name, date, firing, wet, dry and fired lengths for every test bar.
Worked examples, practical checks and limitations
- Use the clay maker’s data sheet as a starting point, then confirm with your own test bar.
- Fire the test bar in the same kiln and schedule as your real work.
- Test at the target temperature and one cone above and below, so you can see how shrinkage and density change near your firing point.
- Glazes, warping and uneven drying are not included in the arithmetic.
- Soil-science texts sometimes divide by dry length; a figure from such a source is not directly comparable.
Common mistakes and when to seek expert confirmation
The classic mistake is adding the percentage to the target size. Others are mixing shrinkage measured at different firing temperatures and trusting a number for a different clay body. For lids, fitted parts and commissions, fire a test first or ask your clay supplier.
Frequently asked questions
How big should I make pottery before firing?
Divide the fired size you want by the shrink factor. With 12% shrinkage, 200 ÷ 0.88 = 227.27 mm.
Why did my pot come out smaller than planned?
Often the percentage was added to the target instead of dividing by the shrink factor, or the clay shrinks more than the number used.
Where do I find my clay’s shrinkage?
On the clay maker’s data sheet, or by measuring a test bar.
Does shrinkage apply to height and thickness too?
Yes, to every linear dimension.
Can I add the drying and firing percentages?
No. Measure wet to fired directly, or multiply the stage factors (0.94 × 0.9309 ≈ 0.875 in the example).
Why fire test bars at more than one temperature?
Shrinkage and absorption change with temperature, and a clay can be overfired if your kiln runs hot. Bars one cone above and below your target show how safe your firing point is.
Conclusion
Measure your clay, divide by the shrink factor and record every test. A few test bars save many ruined pots.
Sources
- Digitalfire: SHAB shrinkage and absorption test
- Digitalfire: Making test bars for the SHAB, LDW and DFAC tests
- Digitalfire glossary: Firing shrinkage
- Digitalfire: Simple physical testing of clays

Share Your Opinion